Partial discharge ceramic substrates must be designed so the operating voltage stays well below the PD inception voltage (PDIV)—the point where localised gas ionisation begins inside voids, delaminations, or at metallisation edges. For 96 % Al₂O₃ substrates 0.63 mm thick, PDIV usually falls between 4 kV and 8 kV AC rms (per IEC 60270 at 50 Hz), depending on metallisation quality, surface roughness, and edge geometry. Designing below PDIV is the single most important factor for long-term insulation life in traction inverters, SiC gate drivers, and industrial power supplies rated above 1 200 V.

Partial discharge is a localised ionisation event that occurs in a region of the insulation where the electric field exceeds the breakdown strength of the gas filling a defect, but does not bridge the full insulation thickness. Each PD event deposits a tiny amount of energy—on the order of picojoules—into the ceramic surface. Over millions of cycles at power-line or switching frequencies, this energy erodes the grain boundaries of the ceramic, eventually forming conductive carbon tracks or micro-cracks that lead to full dielectric failure.
In a power module, the ceramic substrate is the primary electrical insulation between the high-voltage die and the grounded baseplate. If PD activity exceeds roughly 10 pC (the common acceptance threshold in IEC 61287-1 for railway traction), the substrate’s expected life drops dramatically. A substrate that passes a 10 kV hipot test can still fail in service if PD is active at the operating voltage—hipot confirms no puncture, but says nothing about partial discharge ceramic degradation.
PDIV depends on the substrate material, thickness, metallisation process (DBC vs. AMB), surface finish, and the geometry of conductor edges. The table below gives representative ranges measured per IEC 60270 at 50 Hz on commercially available substrates.
| Parameter | Al₂O₃ 96 % | AlN | Si₃N₄ | Unit | Condition |
|---|---|---|---|---|---|
| Dielectric strength (bulk) | 12–17 | 14–17 | 15–20 | kV/mm | ASTM D149, 20 °C, DC |
| Typical substrate thickness | 0.38–1.0 | 0.63–1.0 | 0.32–0.64 | mm | — |
| PDIV (DBC, standard edge) | 4–8 | 6–10 | 8–15 | kV AC rms | IEC 60270, 50 Hz, 20 °C |
| PDIV (AMB, optimised edge) | 6–10 | 8–13 | 10–18 | kV AC rms | IEC 60270, 50 Hz, 20 °C |
| Flexural strength | 300–380 | 300–400 | 600–900 | MPa | ASTM C1161, 3-pt bend |
| Fracture toughness K_IC | 3.5–4.0 | 2.5–3.5 | 5–7 | MPa·√m | ASTM C1421 |
Typical values for commercially available material, for comparison only. Confirm against the datasheet for your specific grade. Sources: CoorsTek ADS-996 datasheet; Kyocera SN-220 datasheet; Rogers curamik AMB product guide.
Si₃N₄ stands out for two reasons. First, its higher flexural strength and fracture toughness mean that even if PD-induced micro-cracks initiate, they propagate more slowly. Second, AMB (active metal brazing) on Si₃N₄ produces a smoother, better-bonded copper edge than DBC on Al₂O₃, reducing the field enhancement that triggers partial discharge. This is why most 3.3 kV and 6.5 kV SiC module platforms—such as those documented in Infineon’s application notes for the FF600R07ME4—specify Si₃N₄ AMB substrates.
PD almost never initiates in the bulk ceramic. The two dominant initiation sites are:
1. Metallisation edges. The copper trace terminates with a sharp geometric discontinuity. The electric field at this edge can be 2–5× the average field across the substrate thickness. On a DBC substrate, the copper is bonded by a eutectic Cu-O layer, and the etch process leaves a ragged edge profile. AMB substrates use a sputtered or screen-printed Ti/Ag/Cu braze, which can be laser-trimmed to a controlled edge angle—typically 20–40° from horizontal—reducing field concentration.
2. Internal voids and delaminations. Gas pockets between the copper and ceramic, or within the braze layer, act as capacitors in series with the ceramic. Because the gas has a lower permittivity (~1.0) than the ceramic (~9–10 for Al₂O₃), the voltage across the void is disproportionately high. A 50 µm void in a 0.63 mm Al₂O₃ substrate operating at 5 kV sees a local field of roughly 8–10 kV/mm across the gas gap—well above the ~3 kV/mm Paschen breakdown threshold for air at that gap distance.
Consider a 0.63 mm thick AlN DBC substrate with 0.3 mm copper. The system voltage is 3.3 kV DC (equivalent to ~2.3 kV AC rms for a 50 Hz sinusoidal test). The average field across the ceramic is:
E_avg = 3 300 V / 0.63 mm = 5.24 kV/mm
At a copper edge with a 90° termination angle, FEM simulations (published by Fraunhofer IISB, 2019) show a field enhancement factor of 2.5–3.5×. Taking 3× as a mid-range estimate:
E_edge ≈ 3 × 5.24 = 15.7 kV/mm
This exceeds the bulk dielectric strength of AlN (14–17 kV/mm per ASTM D149). PD will initiate at the edge well before bulk breakdown occurs. If the edge is chamfered to 30° via AMB laser trimming, the enhancement factor drops to ~1.5–2×, giving E_edge ≈ 7.9–10.5 kV/mm—below the bulk strength and likely below PDIV for this thickness.
This example explains why creepage and clearance rules for ceramic substrates must account for field enhancement, not just linear distance.
Enter your substrate thickness, material, and system voltage below to estimate the derating margin relative to PDIV for your partial discharge ceramic design.

For system voltages above 1 700 V, specify Si₃N₄ AMB. For 1 200 V-class modules, AlN DBC at 0.63 mm is usually sufficient if edge geometry is controlled. Al₂O₃ works for ≤600 V applications or where cost is the primary driver. Increasing substrate thickness raises PDIV roughly linearly, but also increases thermal resistance—a direct trade-off. A ceramic PCB designed for SiC power modules typically balances 0.32 mm Si₃N₄ with AMB edge control rather than using a thicker, thermally inferior substrate.
Specify a copper setback (the distance from the copper edge to the substrate edge) of at least 0.8–1.2 mm for 3.3 kV-class designs. For AMB substrates, request a controlled braze fillet angle of ≤40° from horizontal. Some manufacturers offer a dielectric coating (e.g., polyimide or silicone gel fill) over the copper edge to replace the air gap with a higher-permittivity medium, raising PDIV by 20–40 %.
Specify void content in the bond layer by ultrasonic scanning (C-SAM). A common acceptance criterion is <2 % void area per die-attach zone. For the substrate bond itself, <1 % total void area is achievable with AMB on Si₃N₄. DBC on Al₂O₃ typically yields 1–3 % void area. Each void is a potential PD site.
Derate the continuous operating voltage to ≤70 % of the measured PDIV. For a substrate with a PDIV of 10 kV AC rms, this means a maximum operating voltage of 7 kV AC rms. This 70 % rule is consistent with IEC 61287-1 for traction converters and with Infineon’s and Wolfspeed’s power module design guidelines.
Proper manufacturing process control also matters: if copper registration shifts toward the substrate edge, the effective setback shrinks and PDIV drops.
PD testing per IEC 60270 requires a shielded measurement setup with background noise below 1–2 pC. The substrate is placed between electrodes, voltage is ramped at 50 Hz or 60 Hz, and the PD inception voltage (where PD first exceeds the detection threshold, usually 5 or 10 pC) and PD extinction voltage (where PD drops below threshold on voltage ramp-down) are recorded. The difference between PDIV and PDEV indicates hysteresis in the discharge sites.
For production screening, many power module manufacturers test at 1.5× or 2× the rated operating voltage for 10 seconds with a PD threshold of 10 pC. Substrates that exceed this threshold are rejected. If you are designing a multilayer ceramic PCB for a high-voltage application, PD testing must be performed on each insulation layer independently, since internal vias and buried conductors create additional field concentration points.
If your system voltage is below 600 V DC and the substrate operates in a silicone-gel-encapsulated environment, PD is unlikely to be the life-limiting failure mode. Thermal cycling fatigue, solder joint cracking, and wire bond lift-off will dominate. In these cases, standard Al₂O₃ DBC with a basic hipot test is sufficient. FR-4 or metal-core PCBs may also be adequate for low-voltage, low-power designs where ceramic’s cost premium is not justified. PD-focused design adds cost through tighter edge tolerances, AMB processing, and C-SAM inspection—spend that budget only when the voltage demands it.
Yes. Sustained PD erodes grain boundaries and creates conductive surface tracks over thousands of operating hours. The substrate does not fail immediately—PD is a slow degradation mechanism—but it eventually leads to full dielectric breakdown. The time to failure depends on PD magnitude, frequency, and the ceramic’s fracture toughness.
Most industry standards (IEC 61287-1, Infineon and Wolfspeed application notes) specify a PD threshold of ≤10 pC at the rated test voltage. Some automotive OEMs require ≤5 pC. Below these levels, PD-induced degradation is negligible over a 20-year service life.
Silicone gel encapsulation raises PDIV by 30–60 % compared to air, because the gel fills surface voids and has a higher dielectric strength (~15–20 kV/mm) than air. However, gel does not eliminate PD from internal voids within the bond layer, so void-free bonding remains essential.
No. Hipot (dielectric withstand) testing applies a high voltage and checks for full breakdown or excessive leakage current. PD testing, per IEC 60270, measures small discharge pulses in the picocoulomb range at lower voltages. A substrate can pass hipot and still have active PD that shortens its life.
Elevated temperature increases PD activity. The dielectric strength of trapped gas decreases as temperature rises (per Paschen’s law at reduced gas density), and thermal expansion can open micro-gaps at bond interfaces. PDIV measured at 150 °C is typically 10–20 % lower than at 25 °C. Always test and derate at the maximum expected operating temperature.
If you are designing a partial discharge ceramic substrate for a power module rated above 1 200 V, start by defining your required PDIV based on system voltage and derating rules, then select the ceramic material and metallisation process to meet it. For substrate sourcing or design review support, request a quote from AluminaPCB with your voltage class, substrate dimensions, and copper layout.
Last reviewed: 2025-07