A ceramic PCB is the preferred substrate for solid-state relays (SSRs) rated above 400 V or dissipating more than 2–3 W per channel because it combines high dielectric strength (≥ 15 kV/mm for 96 % Al₂O₃), tight creepage control on a flat surface, and thermal conductivity 10–20× better than FR-4. This guide to ceramic PCB design for solid state relay applications covers material selection, creepage and clearance layout, thermal design, and a worked sizing example for a 600 V / 10 A SSR module.

A solid-state relay switches mains or DC bus voltage using MOSFETs, thyristors, or IGBTs. The control side is galvanically isolated from the load side, and the substrate must maintain that isolation under surge and partial-discharge conditions. FR-4 has a dielectric strength of about 20 kV/mm in theory, but moisture absorption, glass-weave voids, and resin degradation above 130 °C reduce it in practice. Ceramic is dimensionally stable, non-hygroscopic, and rated for continuous use well above 300 °C.
Thermal performance matters because SSR on-state losses scale with I²·RDS(on). A 10 A MOSFET with 80 mΩ RDS(on) dissipates 8 W at full load. On a 1.6 mm FR-4 board (0.25 W/mK), the substrate thermal resistance alone would be roughly 40 °C/W for a 10 × 10 mm footprint. On 0.635 mm 96 % alumina (25 W/mK), that drops to about 2.5 °C/W — a 16× improvement that directly lowers junction temperature. This is why ceramic PCB design for solid state relay applications dominates in high-power, high-voltage modules.
| Parameter | Al₂O₃ 96 % | Al₂O₃ 99.6 % | AlN | Unit | Condition | Source |
|---|---|---|---|---|---|---|
| Thermal conductivity | 24–28 | 28–33 | 170–200 | W/mK | 25 °C | CoorsTek / Maruwa datasheets |
| Dielectric strength | ≥ 15 | ≥ 17 | ≥ 15 | kV/mm | ASTM D149, 60 Hz | Kyocera technical ceramics catalog |
| CTE | 7.2 | 7.1 | 4.5 | ppm/K | 25–400 °C | CoorsTek |
| Flexural strength | 345 | 380 | 300–350 | MPa | ASTM C1161 | CeramTec |
| Volume resistivity | > 10¹⁴ | > 10¹⁴ | > 10¹⁴ | Ω·cm | 25 °C | Kyocera |
| Relative cost index | 1× | 1.3–1.5× | 3–5× | — | — | Industry pricing |
Typical values for commercially available material, for comparison only. Confirm against the datasheet for your specific grade.
For the majority of SSR modules rated 400–1200 V and dissipating under 15 W total, 96 % alumina with DBC or DPC metallization is the cost-effective choice. Reserve AlN for designs where the die sits directly on the substrate and thermal flux density exceeds 30 W/cm², such as SiC MOSFET-based SSRs in compact packages. Material selection is the first decision in any ceramic PCB design for a solid state relay, and getting it right avoids costly respins.
IEC 60664-1 defines minimum creepage distances based on the working voltage, pollution degree, and the comparative tracking index (CTI) of the substrate material. Ceramics fall into Material Group I (CTI ≥ 600 V), which allows the shortest creepage for a given voltage. For a 600 Vrms working voltage at Pollution Degree 2, IEC 60664-1 Table F.4 specifies a minimum creepage of 6.3 mm on Material Group I substrates.
On a ceramic PCB, the flat, non-porous surface means creepage distance equals the physical gap between copper features — no derating for surface roughness or absorbed moisture. This is a real advantage over FR-4, where solder mask quality and laminate texture introduce uncertainty. When laying out your SSR, place the control-side copper and load-side copper on opposite ends of the substrate with a bare ceramic channel between them. Avoid routing traces that reduce the effective creepage path around corners.
For designs requiring reinforced insulation per IEC 62368-1 or IEC 60950-1, double the basic creepage or use a thicker substrate (≥ 1.0 mm) to meet the through-substrate clearance requirement simultaneously. Consult the ceramic PCB design guidelines for minimum feature sizes that affect achievable gap widths.
600 V / 10 A single-phase SSR using two anti-parallel SCRs. Each SCR dissipates 6 W at rated current (VT ≈ 1.2 V × 5 A average per half-cycle). Total substrate dissipation: 12 W. Maximum ambient: 85 °C. Target case temperature under the substrate: ≤ 125 °C.
Using a 0.635 mm thick, 25 × 20 mm 96 % alumina substrate (k = 25 W/mK):
Rθ,sub = t / (k × A) = 0.000635 / (25 × 0.0005) = 0.051 °C/W
The substrate itself contributes negligible resistance. The dominant terms are the die-attach layer (typically 0.3–0.8 °C/W for solder, 2–5 °C/W for adhesive) and the substrate-to-heatsink interface (0.5–2.0 °C/W depending on thermal grease and clamping pressure).
Enter your substrate dimensions, thickness, and total dissipated power below to estimate junction-to-case temperature rise for your own ceramic PCB design solid state relay layout.
Assuming solder die-attach (0.5 °C/W) and a thermal pad interface (1.0 °C/W):
ΔT = 12 W × (0.5 + 0.051 + 1.0) = 18.6 °C
Case temperature = 85 + 18.6 = 103.6 °C — well within the 125 °C target. On FR-4 the substrate term alone would add 48 °C, blowing the budget. For more on ceramic thermal management strategies, including heatsink attachment methods, see the dedicated guide.

DBC (direct bonded copper) bonds 0.15–0.30 mm copper foil to alumina at high temperature, giving excellent current-carrying capacity for the load-side traces. DPC (direct plated copper) builds copper layers by sputtering and electroplating, achieving finer features (trace/space down to 50 µm or less) for the control-side circuitry. Many SSR substrates use DBC on one side for power and DPC on the other for signal routing. Selecting the right process is a critical step in ceramic PCB design for solid state relay substrates.
Thick-film gold or silver metallization is another option when wire bonding to die. The choice depends on your assembly process: if you solder packaged MOSFETs, DBC/DPC copper with ENIG finish works. If you bond bare die, thick-film gold pads provide reliable Au-Au or Au-Al wire bonds. Review the ceramic PCB manufacturing process overview to match your assembly method to the right metallization technology.
Ceramic substrates add cost — typically 5–15× the bare-board price of FR-4 for equivalent area. They are also brittle and require careful handling during assembly. Consider alternatives in these situations:
For a broader comparison of substrate options and their ceramic PCB cost drivers, see the cost breakdown page.
Yes. A ceramic substrate with adequate creepage (per IEC 60664-1) and a high-voltage-rated die provides galvanic isolation without an optocoupler. Many modern SSR designs use capacitive or magnetic isolation ICs on the control side and power MOSFETs on the load side, all mounted on one ceramic board.
ENIG (electroless nickel / immersion gold) over DPC or DBC copper is the most common choice. It provides a solderable, oxidation-resistant surface compatible with SAC305 and other lead-free solders. For high-reliability applications, ENEPIG adds a palladium barrier layer.
Ceramic substrates tolerate standard reflow profiles (peak 260 °C for SAC305) without damage. The risk comes from rapid thermal shock — ramp rates above 4–5 °C/s can stress thin substrates (≤ 0.38 mm). Follow the substrate manufacturer’s recommended profile, and avoid placing cold boards directly onto a hot belt.
Partial discharge (PD) testing per IEC 60270 is required for reinforced insulation in many safety standards. Ceramic substrates generally exhibit PD inception voltages well above 1 kVpk for 0.635 mm alumina, but the metallization pattern edges and solder fillets can be initiation sites. Keep copper edges smooth, avoid sharp internal corners, and specify PD testing at 1.5× working voltage during qualification.
96 % alumina substrates are rated for continuous use above 800 °C in air. The practical limit for an SSR is set by the solder joints and semiconductor die, not the ceramic. With standard SAC305 solder, the assembly limit is around 150 °C; with high-temperature solder (e.g., AuSn) or sintered silver die-attach, operation up to 250–300 °C is feasible. For more on ceramic PCB maximum operating temperature, see the dedicated article.
If you are designing a ceramic substrate for a solid-state relay, prepare your creepage requirements, load current, and thermal budget, then request a design review and quote. An applications engineer can confirm material grade, metallization process, and achievable tolerances for your specific SSR layout.