A cavity ceramic PCB is a substrate with one or more pockets machined or laminated into its surface so that a bare die, sensor, or discrete component sits recessed below the top plane. Recessing the die shortens wire-bond loops by 0.1–0.5 mm, reduces package height, improves the thermal path to the backside, and provides a shelf for hermetic lid or cap sealing. Cavity structures are standard practice in HTCC and LTCC processes and can also be formed by laser or mechanical milling in fired alumina and aluminum nitride substrates.

The fabrication method depends on whether the ceramic is processed before or after sintering. Each approach carries different tolerance, cost, and geometry trade-offs.
In co-fired processes, individual tape layers are punched or laser-cut with windows before lamination. Stacking layers with progressively larger or smaller windows creates the cavity or step profile. Because the cavity forms before sintering, the shrinkage of the ceramic (12–16 % for LTCC, 15–20 % for HTCC) must be accounted for in the punch dimensions. Depth resolution equals the fired layer thickness, typically 50–200 µm per layer for LTCC and 100–300 µm for HTCC. This method is the lowest-cost route for high volumes because no secondary machining is needed.
Fired alumina (96 % or 99.6 %) and AlN substrates can be milled with diamond tooling or ablated with a CO₂ or UV laser. Post-fire machining offers freeform cavity shapes and depth control independent of layer count, but it is slower and more expensive per unit. Surface roughness after laser ablation is typically Ra 1–3 µm; diamond grinding can achieve Ra < 0.5 µm where a smooth die-attach surface is required.
Single-layer substrates made by DPC (direct plated copper) do not inherently support cavities. A pseudo-cavity can be created by bonding a frame or ring of ceramic onto the base substrate, but this adds an assembly step and an additional interface. For true cavity structures, co-fired or post-fire machined substrates are preferred.
| Structure | Description | Typical Use |
|---|---|---|
| Simple cavity (pocket) | Single rectangular or circular recess, one depth | Single bare-die attach, MEMS sensor housing |
| Step cavity | Two or more shelves at different depths within one opening | Wire-bond landing pad at an intermediate level; stacked die |
| Through cavity | Window cut entirely through the substrate | Optical path, air-flow channel, backside access for flip-chip |
| Blind trench / slot | Narrow elongated recess, not full pocket | RF isolation, thermal break, fiber alignment groove |
Typical values for commercially available material, for comparison only. Confirm against the datasheet for your specific grade.
Getting a cavity design through fabrication without cracking, warping, or delamination requires attention to several geometric constraints. The table below summarizes typical limits; your fabricator’s specific capability sheet supersedes these ranges.
| Parameter | LTCC (green-tape) | HTCC (green-tape) | Post-fire machined (Al₂O₃ / AlN) | Unit |
|---|---|---|---|---|
| Min wall thickness | 0.3–0.5 | 0.5–0.8 | 0.4–0.6 | mm |
| Depth tolerance | ±25–50 per layer | ±30–50 per layer | ±20–30 absolute | µm |
| Max depth / substrate thickness | ~65 % | ~60 % | ~70 % | ratio |
| Min corner radius (internal) | 0.15 | 0.2 | 0.1 (laser) | mm |
| Floor flatness | ≤ 25 µm over 5 mm | ≤ 30 µm over 5 mm | ≤ 10 µm (ground) | µm |
| Positional tolerance (cavity to pad) | ±50 | ±75 | ±25 | µm |
Ranges compiled from published LTCC/HTCC design guides by Kyocera, CoorsTek, and CeramTec. Confirm against your fabricator’s capability document.
A few rules that prevent the most common rejections during Review ceramic PCB drawing requirements:
Suppose you are mounting a 0.1 mm thick GaN die into a 1.0 mm thick LTCC substrate. The die-attach solder or epoxy adds 0.025 mm. You want the die top surface flush with the substrate surface for short wire bonds to pads on the top layer.
Required cavity depth = substrate thickness − (die thickness + attach layer) = 1.0 − (0.1 + 0.025) = 0.875 mm.
At 0.875 / 1.0 = 87.5 % of substrate thickness, this exceeds the ~65 % guideline. The floor would be only 0.125 mm thick, risking cracking. Two solutions:
Option 1 is preferred when package height allows it. Option 2 is a compromise for height-constrained designs. In either case, verify the cavity floor flatness requirement against the die-attach process spec.

Any ceramic that can be co-fired or machined can host a cavity, but the choice affects achievable wall thickness and thermal performance.
For multilayer ceramic builds, LTCC and HTCC are the natural choices because the cavity forms during lamination at no extra process cost. Single-layer alumina or AlN substrates require post-fire machining, which adds cost but offers tighter depth control.
Cavities add cost, reduce yield, and constrain panelization. Skip them if:
In RF and microwave ceramic designs, cavities serve a dual purpose: housing the MMIC die below the ground plane and creating a controlled electromagnetic environment. The cavity walls act as a partial waveguide boundary, so wall height and width affect resonant modes. Keep cavity dimensions below λ/4 at the operating frequency to avoid parasitic resonances. For a 30 GHz design in LTCC (εr ≈ 7.1), λ/4 ≈ 0.94 mm — tight, but achievable with careful layout.
Yes. Both co-fired and post-fire processes support metallized cavity floors for die attach, ground planes, or signal routing. In co-fired processes, the metal is printed on the green tape before lamination. For post-fire machined cavities, the floor is metallized after machining using thin-film sputtering or thick-film screen printing. Ensure the metal setback from the cavity wall is at least 0.1 mm to avoid edge cracking.
Practical minimum is about 0.5 × 0.5 mm in LTCC and 1.0 × 1.0 mm in HTCC or post-fire machined alumina. Below these sizes, tooling limitations and inspection difficulty make the feature unreliable. Laser machining can go smaller, but cost per unit rises sharply.
They reduce cross-sectional area, which lowers flexural strength proportionally. A substrate with a cavity occupying 50 % of its thickness has roughly half the bending strength of a solid substrate of the same material. Design the surrounding frame and mounting to minimize bending loads, and follow the reliability design guidelines for ceramic PCBs.
Yes. The shelf or step around the cavity provides a sealing surface for a metal or ceramic lid attached by solder, glass frit, or laser welding. Hermeticity per MIL-STD-883 Method 1014 (fine and gross leak) is routinely achieved with HTCC and LTCC cavity packages. The sealing ring metallization must be continuous and co-planar to within ±10 µm for reliable seam sealing.
The cavity floor thickness is the remaining ceramic between the die and the backside. Thinner floors mean lower thermal resistance. For Al₂O₃ 96 % with a 0.3 mm floor under a 3 × 3 mm die, conduction resistance through the floor is approximately 0.3 / (26 × 9 × 10⁻⁶) ≈ 1.28 °C/W. Halving the floor to 0.15 mm halves that to ~0.64 °C/W, but risks mechanical failure. Balance thermal need against structural limits.
No. A counterbore is a recess around a single via or mounting hole, typically for a screw head or connector pin. A cavity is a larger pocket intended to house one or more components. The design rules overlap, but cavities have stricter wall-thickness and flatness requirements because they carry functional components.
If you are defining a cavity or step structure for your ceramic substrate, review the ceramic DFM checklist to catch common issues before submitting files. When your design is ready, request a quote with your cavity drawing and we will confirm achievable tolerances for your specific geometry.